Example of Tirneauuz tungsten-molybdenum ore dressing plant in the Caucasus

    1 Introduction
    Located in the Caucasus, Tirne Auz is a tungsten- molybdenum mining-selection joint venture.
    1940 flotation production, the existing production capacity of 1200t / d, the amount of molybdenum is a gold production per year 3000t, tungsten metal content 2400t.
    2. Deposits, ores and mining
    Tierne Auz is a skarn or skarnized marble molybdenum-tungsten deposit and horn rock and granite molybdenum deposit. The proven ore reserves are 50 Mt, the tungsten and molybdenum grades are 0.65% WO 3 and 0.25% Mo, and the retained molybdenum metal reserves are 125 kt, of which the recoverable molybdenum metal is 65 kt.
    The ore is classified into two types, silicate and carbonate, according to the type of associated gangue.
    The main metal minerals in the skarn type ore are fine-grained inlaid (0.01~lmm) scheelite , tungsten-molybdenum-calcium ore and molybdenum ore present in surrounding rocks (hornblende, garnet, quartz, etc.). The ore has the highest content of molybdenum and tungsten trioxide. There are also copper , bismuth , gold, silver , selenium , hooves, fluorite and the like.
    The distribution of molybdenum-containing minerals and molybdenum in the ore is: molybdenum ore 50%, molybdenum-tungsten ore 30%, molybdenum-containing scheelite 11%, and molybdenum-containing vermiculite 8%.
    Mine used pit mining, crushing the stope, ore dressing plant with ropeway sent.
    3. Mineral processing technology
    Tierne Uz tungsten-molybdenum ore comprehensively recovers molybdenum, copper and tungsten, using copper-molybdenum mixed flotation; copper-molybdenum separation and copper selection; copper-molybdenum mixed flotation tailings flotation scheelite.
    The copper-molybdenum mixed flotation and copper-molybdenum separation process is shown in Figure 1. The copper-molybdenum mixed float is selected from coarse grinding (60%~69%-200 mesh), one rough selection, one sweep selection, and two selective processes. The copper-molybdenum mixed concentrate was subjected to steaming heat treatment and a section (three fine bubbles) for re-grinding, and five times (third to seventh) were selected to obtain qualified molybdenum concentrate. After the copper-molybdenum sorting ore is mixed and floated, it is subjected to steaming heat treatment and molybdenum floating copper to obtain qualified copper concentrate.
    Figure 1 Tirne Auz selection plant process
    [next]
    The process of the tungsten recovery circuit is shown in Figure 2. The sulphur concentrate is divided into three streams: the first one enters re-selection to obtain high-grade scheelite concentrate; the second one directly leaches phosphorus ; the third one is low-quality scheelite concentrate, which is sent to the water and metallurgical plant for treatment.
    The white tungsten coarse concentrate is selected by steaming process, and the slurry is heated to 85~87 °C, and then treated with 2.7%~3% water glass solution for 60 min and then selected.
    Figure 2 Tirne Auz recycling white tungsten process
    4. Mineral processing agent
    The mineral processing agent system is listed in the table below.
    Table Tierner Auze Concentrator Pharmacy System
    Work
    Calcined soda
    Butyl xanthate
    Fatty acid
    Transformer oil
    Coal oil
    Isodecenol
    Sodium sulfide
    Sodium cyanide
    Water glass
    Grinding
    690
    5
    Molybdenum rough selection
    5
    50
    Regrind
    6
    Molybdenum selection
         
    50
    50
    5
    130
    Copper-molybdenum ore flotation:
    Mixed rough selection
    0.7
    2
    2
    Sweep
    0.3
    30
    Stir
    350
    White tungsten flotation:
    Rough selection
    40
    41
    Sweeping (I and II)
    27
    I selection
    150
    Steam heating
    1880
    Total consumption
    730
    10
    68
    10
    52
    48
    80
    5
    2516
    5, mineral processing indicators
    The ore grade is 0.65% Mo, 0.25% WO 3 ; the ore processing capacity is 1200t/d, the grinding fineness is 60%-200 mesh; the molybdenum concentrate grade is 47.65% Mo, 0.416% WO 3 , the molybdenum recovery rate is 47.98%; The ore grade is 61.94% WO 3 , 3.56% Mo, the tungsten recovery rate is 22.23%; the white tungsten intermediate product grade is 44.41% WO 3 , 3.59% Mo, the tungsten recovery rate is 62.79%; the power consumption is 18.56kW·h/t ore, water: 2.208 m 3 /t mine, steel ball: 0.855kg / t mine, liner: 0.lkg / t mine.

    Road Machinery

    Our Road Machinery includes Concrete Mixer,Road roller,Sprinkler,Road sweeper.It is all the machinery needed in the whole road construction and maintenance.

    Road Machinery,Small Construction Mixer Cement,Water Sprinkler Truck,Ntelligent Street Ride Sweeper

    Jiangsu Minnuo Group Co.,Ltd , https://www.js-minnuomachinery.com

    Previous Post: LED industry enters stable income era from excessive competition
    Next Post: Cabinet Doors and Cable Seal Container Seal Cutter Rubber Seal
    Home
    Recent Posts
    • Yqw-02g Propane Regulator with High Quality
    • Manufacture High Quality Wire Mesh Mist Eliminat…
    • New probes for mitochondrial autophagy process d…
    • Ozone System for Drinking Water Plant Water Trea…
    • The sales volume of hot-selling SUVs in the four…
    • Yolink Pneumatic Solenoid Valve
    • Two Waves 3mm Material Thickness Highway Guardra…
    • Toyota Car Flang Chrome Wheel Lug Nuts
    • Teflons Coated Heavy Hex Nuts and Flat Washers
    • Agricultural Farm/Garden Mini Tractor Power Till…
    • High Capacity Oil Centrifuge (LW1100X4400)
    • The South Pump Industry builds China's pump …
    • Laser lithography system pulse width broadening …
    • China Supplier Stainless Steel 7.5HP Water Pump
    • Screw Type Water Cooled Industrial Water Chiller
    • Chinese Engines and Engine Parts for Sale
    • Yantai Automobile Parts Exports Increased by 24.…
    • Chevrolet Luv Pickup & Isuzu Pickup Auto Starter…
    • The Seventh Symposium on the Application of Risk…
    • Chipboard Screw Yellow Blue White Zinc 5*35